Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® T KR 4355 G10 bk 23215 - PA6T/6-GF50 - BASF

Material Data Center offers the following functions for Ultramid® T KR 4355 G10 bk 23215:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Ultramid T datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
玻璃纤维增强注塑等级。 具有高韧性、 刚度和强度、 低吸水性、 高熔点(295 °C)。 材料精加工后, 其机械性能在60 °C以下保持稳定。
加工/物理特性干 / 已调节单位Test Standard
ISO数据
模塑收缩率, 平行 0.2 / * % ISO 294-4, 2577
模塑收缩率, 垂直 0.7 / * % ISO 294-4, 2577
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 17000 / 16000 MPa ISO 527
断裂应力 240 / 190 MPa ISO 527
断裂伸长率 2.4 / 2.5 % ISO 527
拉伸蠕变模量, 1000h * / 10500 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 90 / 80 kJ/m² ISO 179/1eU
简支梁冲击强度, -30°C 85 / 75 kJ/m² ISO 179/1eU
简支梁缺口冲击强度, +23°C 13 / - kJ/m² ISO 179/1eA
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 285 / * °C ISO 11357-1/-3
热变形温度, 1.80 MPa 245 / * °C ISO 75-1/-2
线性热膨胀系数, 平行 18 / * E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 55 / * E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 1.6 / * mm -
Yellow Card 现存 是的 / * - -
厚度为h时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 1.6 / * mm -
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 1MHz 4.7 / 4.8 - IEC 62631-2-1
介质损耗因子, 1MHz 200 / 300 E-4 IEC 62631-2-1
体积电阻率 >1E13 / >1E13 Ohm*m IEC 62631-3-1
表面电阻率 * / >1E15 Ohm IEC 62631-3-2
介电强度 33 / 31 kV/mm IEC 60243-1
相对漏电起痕指数 - / 600 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 4 / * % 类似ISO 62
吸湿性 0.6 / * % 类似ISO 62
密度 1620 / - kg/m³ ISO 1183
模塑测量的特殊性能干 / 已调节单位Test Standard
ISO数据
粘数 135 / * cm³/g ISO 307, 1157, 1628
试样制备条件价值单位Test Standard
ISO数据
注塑, 熔体温度 320 °C ISO 294
注塑, 模具温度 100 °C ISO 294
加工推荐(注塑)价值单位Test Standard
预干燥-温度 110 °C -
预干燥-时间 8 h -
加工湿度 ≤0.15 % -
注塑熔体温度 310 - 330 °C -
模具温度 80 - 120 °C -
函数
应力-应变.  , Ultramid® T KR 4355 G10 bk 23215 (烘干), PA6T/6-GF50, BASF
应力-应变.  , Ultramid® T KR 4355 G10 bk 23215 (状况), PA6T/6-GF50, BASF
正割模量-应变.  , Ultramid® T KR 4355 G10 bk 23215 (烘干), PA6T/6-GF50, BASF
正割模量-应变.  , Ultramid® T KR 4355 G10 bk 23215 (状况), PA6T/6-GF50, BASF
应力-应变(等时的) 23°C, Ultramid® T KR 4355 G10 bk 23215 (状况), PA6T/6-GF50, BASF
蠕变模量-时间. 23°C, Ultramid® T KR 4355 G10 bk 23215 (状况), PA6T/6-GF50, BASF
蠕变曲线 23°C, Ultramid® T KR 4355 G10 bk 23215 (状况), PA6T/6-GF50, BASF
拉伸模量-温度 , Ultramid® T KR 4355 G10 bk 23215 (烘干), PA6T/6-GF50, BASF
拉伸模量-温度 , Ultramid® T KR 4355 G10 bk 23215 (状况), PA6T/6-GF50, BASF
典型数据
加工方法
注塑
供货形式
黑色
地区供应
其他信息
注塑成型
PREPROCESSING
Pre/Post-processing, max. allowed water content: .15 %
Pre/Post-processing, Pre-drying, Temperature: 110 °C
Pre/Post-processing, Pre-drying, Time: 8 h

PROCESSING
injection molding, Melt temperature, range: 310 - 330 °C
injection molding, Melt temperature, recommended: 320 °C
injection molding, Mold temperature, range: 80 - 120 °C
injection molding, Mold temperature, recommended: 100 °C
injection molding, Dwell time, thermoplastics: 5 min
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com